ukrabraziv.com — Ukraine's abrasive tools portal
Home›Handbook›Crystal structure and properties of abrasive grain
MaterialsUpdated: October 2026

Crystal structure and properties of abrasive grain

The cutting properties of an abrasive are determined by how the atoms in its crystal are bonded. The shorter and stronger the bonds, the higher the hardness. But hardness alone is not enough for work in a wheel: the grain must be tough enough not to break up under impact and friable enough to fracture and form new edges.

MaterialLatticeMicrohardness, GPaDensity, g/cm³Thermal stability in air, °C
Fused aluminaTrigonal (α-Al₂O₃)19–243.9–4.0up to 1700
Silicon carbideHexagonal32–363.21300–1400
Boron carbideRhombohedral40–452.5500–700
Cubic boron nitrideCubic80–903.45–3.491200–1400
DiamondCubicabout 1003.5700–800

Hardness

The general rule: the abrasive must be at least one and a half to two times harder than the material being machined. Hardened steel has a microhardness of 7–8 GPa, and fused alumina copes with it easily. The carbides in high-speed steel and cemented carbide have a hardness of 15–25 GPa — right up against that of fused alumina, so here silicon carbide, CBN or diamond is needed.

Toughness and friability

Tough grain withstands high forces and is suited to snagging. Friable grain fractures in small pieces and stays sharp under light loads — it is better for finishing operations and heat-sensitive steels. Among the fused aluminas, toughness decreases from zirconia and brown to white, while monocrystalline alumina combines strength with sharpness.

Grain shape

  • Equiaxed grain, close to a cube or a sphere, is stronger and packs densely. It is used in wheels for heavy-duty work.
  • Platy and needle-shaped grain is sharper but breaks more easily. It is preferred for coated abrasives, where the grains are oriented point upwards.

Shape is assessed by bulk density: the higher it is for a given grit size, the more equiaxed the grain.

Microstructure

A grain of fused alumina is a fragment of a large crystal. As it wears, a flat forms on it, and only then does it fracture. A grain of sintered microcrystalline alumina consists of a multitude of crystallites smaller than a micrometre: it sheds them one at a time and stays sharp far longer. The same principle is used in polycrystalline diamond and CBN.

Chemical resistance

Hardness is measured at room temperature, but the grain works at hundreds of degrees. Under these conditions chemistry is decisive: diamond and silicon carbide react with iron, and fused alumina with titanium. That is exactly why the hardest abrasive is not always the best.

This article is for reference only. Check operating parameters and specifications against the documentation of the tool and machine manufacturer.